Quick Order
 
History | Show Schedule | W.R.COBB Guarantee | News | Contact Info
 
 
Master Alloy: W504
Color: White (contains Nickel)
Usage: 18K
Alloy Characteristics 18K
Density (g./cm3)
14.54
Hardness – As Cast (Hv)
225
Hardness – Cold Worked /Reduced 60% (Hv)
>230
Recommended Investment Casting Parameters
18K
Casting Temperature Range (oC)
1065-1100C
Flask Temperature Range (oC)
677-735C
Quench Time (min.)
10-15 min.
Re-alloying Scrap Percentage
<75%
Recommended Cast Tree Cleaning and Drying Procedure

After a preliminary removal of the investment powder during quenching, submerge trees in a hot (80-100oC) 50% phosphoric acid solution for 15-20 minutes. Rinse well with cool water to remove any remaining investment powder and base metal oxides. Dry with compressed air. Do not dry trees in any type of furnace!