Quick Order
 
History | Show Schedule | W.R.COBB Guarantee | News | Contact Info
 
 
Master Alloy: W170
Color: White with Nickel
Usage: 14K and 18K
Material Characteristics 10K 14K
Density
11.50 12.69
Hardness - Cold worked (reduced 60%)
224 Hv 224 Hv
Hardness - Reduced 60%, annealed 15 minutes at 680C, water quenched
195 Hv 190 Hv
Hardness - Reduced 60%, annealed 15 minutes at 680C, air cooled
202 Hv 200 Hv
Investment Casting Parameters
   
Metal Pouring Temperature
1020C 1050C
Quench Time
10-15 min. 10-15 min.