Quick Order
 
History | Show Schedule | W.R.COBB Guarantee | News | Contact Info
 
 
Master Alloy: Y190
Color: Yellow
Usage: 10K, 14K and 18K
Material Characteristics 10K 14K 18K
Density
11.25 12.79 14.86
Hardness - Cold worked (reduced 60%)
228 Hv 228 Hv 228 Hv
Hardness - Reduced 60%, annealed 15 minutes at 680C, water quenched
132 Hv 133 Hv 141 Hv
Hardness - Reduced 60%, annealed 15 minutes at 680C, air cooled
150 Hv 150 Hv 228 Hv
Investment Casting Parameters
     
Metal Pouring Temperature
995C 1010C 1070C
Quench Time
20 min. 20 min. 20min.

© 2011-2012 www.wrcobb.com All Rights Reserved
WR COBB - SERVING INDEPENDENT AND CORPORATE JEWELRY MANUFACTURERS SINCE 1877
USA • HONG KONG • THAILAND • INDIA • BELGIUM • VIETNAM