Quick Order
 
History | Show Schedule | W.R.COBB Guarantee | News | Contact Info
 
 
Master Alloy: Y290
Color: Yellow
Usage: 10K, 14K and 18K
Material Characteristics 10K 14K 18K
Density
11.55 13.11 14.99
Hardness - Cold worked (reduced 60%)
228 Hv 228 Hv 228 Hv
Hardness - Reduced 60%, annealed 15 minutes at 680C, water quenched
200 Hv 195 Hv 144 Hv
Hardness - Reduced 60%, annealed 15 minutes at 680C, air cooled
180 Hv 172 Hv 135 Hv
Investment Casting Parameters
     
Metal Pouring Temperature
995C 1010C 1050C
Quench Time
20 min. 20 min. 20 min.

© 2011-2012 www.wrcobb.com All Rights Reserved